@ARTICLE{Chyrkin:858369,
author = {Chyrkin, A. and Swadźba, R. and Pillai, R. and Galiullin,
T. and Wessel, E. and Grüner, D. and Quadakkers, W. J.},
title = {{S}tability of {E}xternal α-{A}l2{O}3 {S}cales on {A}lloy
602 {CA} at 1100–1200 °{C}},
journal = {Oxidation of metals},
volume = {90},
number = {1-2},
issn = {1573-4889},
address = {Dordrecht [u.a.]},
publisher = {Springer Science + Business Media B.V},
reportid = {FZJ-2018-07255},
pages = {119 - 133},
year = {2018},
abstract = {An external ultrathin α-Al2O3 scale grown on the Ni-base
alloy 602 CA during air oxidation at 800 °C was
characterized by means of high-resolution TEM/EDX and
electron diffraction. Alloy samples pre-oxidized at 800 °C
were subsequently exposed at 1100, 1150 and 1200 °C for up
to 100 h. Whereas the external alumina remained stable at
1100 °C, with the increasing exposure temperature, the
pre-grown alumina scale tended to break down resulting in an
external chromia scale accompanied by internal alumina
precipitation. The transition from external to internal Al
oxidation was investigated using SEM/EDX/EBSD. The critical
Al depletion at the scale-alloy interface during the
post-exposure at 1100–1200 °C was modeled using the
CALPHAD-based thermodynamic-kinetic approach.},
cin = {IEK-2},
ddc = {540},
cid = {I:(DE-Juel1)IEK-2-20101013},
pnm = {111 - Efficient and Flexible Power Plants (POF3-111)},
pid = {G:(DE-HGF)POF3-111},
typ = {PUB:(DE-HGF)16},
UT = {WOS:000437751900007},
doi = {10.1007/s11085-017-9827-0},
url = {https://juser.fz-juelich.de/record/858369},
}